Wesentliche Eigenschaften
- Schrumpfung
- 0.3-0.7 %
- Schmelzen
- 280-20 °C
- Schimmel
- 130-50 °C
- Dichte
- 1.30-.60 g/cm³
- HDT
- 240-80 °C
- Trocknen
- 3 h at 120 °C
Typische Werte für die Materialauswahl. Bitte überprüfen Sie die genaue Materialgüte anhand des technischen Datenblatts (TDS) des Harzlieferanten, bevor Sie ein Werkzeug freigeben oder eine Toleranz festlegen.
Seite an Seite
What PPS actually is
PPS ist ein hochtemperaturbeständiger, teilkristalliner technischer Kunststoff, der für elektrische Bauteile, Automobilteile im Motorraum sowie für Anwendungen eingesetzt wird, die eine hervorragende chemische Beständigkeit und Dimensionsstabilität bei anhaltend hohen Temperaturen erfordern.
Chemically, PPS belongs to the Polyphenylene sulfide - engineering family. The polymer chain structure — linear and semi-crystalline — is what sets its shrinkage behaviour, temperature ceiling and melt flow. Like every thermoplastic, its properties are the result of processing history as much as of the resin grade itself: slow cooling increases crystallinity and brittleness, fast cooling locks in an amorphous structure and a different shrink. Resin suppliers offer PPS in commodity, reinforced and specialty grades, and the first selection step is to pick the right family before settling on a specific TDS.
Bearbeitungsfenster
Run PPS at a melt temperature of 280–320 °C and a mould temperature of 130–150 °C. The high end of the melt range is for thin walls and long flow paths where the resin would freeze before packing; the low end for thick sections where residence time is already long and thermal degradation is the real risk. Above 320 °C the sulphide linkages begin to break, and the first sign is a faint yellow tint and a measurable drop in impact strength rather than a visible surface defect.
The mould temperature is not optional and not optional at the high end. PPS crystallises as it cools, and the mould temperature controls how much crystallinity develops. A mould at 100 °C or lower produces a fast-cooled, low-crystallinity part that looks fine but creeps and softens above 150 °C in service. A mould held at 130–150 °C produces a high-crystallinity part that is dimensionally stable up to 200 °C. Raising mould temperature adds cycle time — roughly 1–2 seconds per 10 °C — and that is why the specification has to include the mould target, not just a part property.
Drying is required. PPS absorbs moisture readily from ambient air, and at 300 °C that moisture reacts with the melt. The visible symptom is silver streaks and burn marks that look like overheat and cannot be fixed by lowering the barrel temperature. Three hours at 120 °C in a desiccant dryer is the normal starting point, and the dew point should be verified at the hopper not at the dryer controller.
Residence time matters as much as temperature. A large barrel running a small shot leaves the melt hot for too long, and the degradation is cumulative — the second shot is more degraded than the first, the tenth more than the second. Size the shot to occupy 40–70 % of the barrel capacity, and purge thoroughly between grades, especially when moving from a lower-temperature commodity to PPS.
Schrumpfung und Maßtoleranz
Entwerfen Sie das Werkzeug so, dass es 0.3–0.7 % shrinkage for unfilled PPS, and up to 0.3 % for glass-filled grades. PPS is semi-crystalline, so flow-direction and cross-flow shrinkage can differ, especially in glass-filled grades where the fibres orientate in the melt flow direction and lock the shrinkage there. That means the correction after first article is not always a uniform offset — it can be directional, and the CMM measurement plan has to cover both directions.
The mould temperature is the single largest influence on crystallinity and therefore on shrinkage. A part cooled in a 140 °C mould develops higher crystallinity and shrinks more uniformly than one cooled in a 100 °C mould, which freezes the amorphous structure and can show warpage. For thin-wall electrical connectors the difference between a 120 °C and a 150 °C mould can decide whether the pin centres fall inside the 0.05 mm tolerance required for a mating fit.
For glass-filled PPS the shrinkage drops to 0.1–0.3 % because the fibres carry the load as the matrix tries to contract. The trade is anisotropy: shrinkage is much lower in flow direction than cross-flow direction on a long thin part. The gate position decides how the fibres align, so the gate has to be placed to minimise the differential, not just to fill the cavity. A side-gated long blade will warp; a centre-gated part keeps the fibre orientation more balanced.
Wir schneiden das erste Muster mit einer Nennzugabe und vermessen die ersten Stücke auf einer Koordinatenmessmaschine, bevor wir den Formhohlraum bearbeiten. Die Korrektur eines Werkzeugs anhand der gemessenen Teile ist kostengünstiger und zuverlässiger als die Korrektur anhand der in den technischen Daten angegebenen Werte, und der Messbericht dient als Ausgangsbasis für das nächste Werkzeug derselben Güteklasse.
What PPS asks of the mould steel
PPS demands three things from the tool at the same time: heat resistance, abrasion resistance and chemical compatibility. That is why its default steel family is H13 / S136, not the P20 that serves commodity resins. A pre-hardened P20 block runs PPS poorly even for short runs, because the mould temperature (130–150 °C) is already close to the tempering temperature of P20 and the block softens and loses polishability quickly.
Die Abrasivität ist Hoch and unavoidable. Glass-filled PPS — the grade most commonly specified — carries 30–40 % glass fibre by weight, and the fibres erode the gate, the vent land and any narrow restriction that increases melt velocity. An unfilled PPS runs low abrasion, but the high-temperature requirement still rules out P20 for anything longer than a prototype campaign. H13 hardened to 48–52 HRC is the default production choice; replaceable gate inserts in DC53 or Vanadis take the brunt of the wear and are cheaper to change than the whole tool.
Chemical attack is Moderate but cumulative. PPS itself is chemically inert, which is why it resists solvents and acids so well. The corrosion comes from additives — flame retardants (brominated or phosphorus-based), lubricants and colourants can release acids at 280–320 °C that corrode carbon steel over thousands of shots. The symptom is not pitting on the cavity surface but a brown discoloration that builds up and transfers to the part, and a die build-up that thickens the vent lands. A passivated S136 stainless block avoids this completely and is the correct choice for any PPS tool that may see FR grades.
Cooling layout has to carry more heat than a commodity tool. PPS runs at 130–150 °C mould temperature, but the melt enters at 280–320 °C, so the heat load is higher than a PP or ABS tool. Baffles and bubblers are not optional on thick sections, and the circuit should run through the gate bushing first since the gate absorbs more heat per unit volume than any other spot in the cavity. Insulate the tool from the platens so the heat stays in the cavity where it belongs, not conducted away by the press.
Applications where PPS wins — and where it gets replaced
PPS occupies the band between commodity engineering resins (PA66+GF, PA46) and ultra-high-temperature resins (PEEK, PES). Its characteristic combination — sustained heat resistance up to 200 °C, excellent chemical resistance to fuels, acids and brake fluids, low creep under load, and a moulded surface that needs little or no post-processing — makes it the default choice for three application families: under-hood automotive electrical components, industrial pump and valve components that see aggressive chemicals, and consumer appliance parts that need heat resistance at moderate stiffness.
The biggest application today is automotive under-hood electrical connectors and housings. These parts need to survive 150 °C continuous service, occasional 180 °C peaks from engine heat, exposure to fuel vapour and road salt, and must hold pin-centre tolerances within ±0.05 mm for the connector mating to work. PA66+GF reaches 150 °C HDT but absorbs moisture and swells — the pin centres shift when humidity changes. PPS does not absorb moisture, so the tolerance holds year round. The tool trade is H13 gate inserts for abrasion and S136 cavity blocks if flame-retardant grades are specified.
PPS gets replaced most often by three alternatives. PA66+GF when the heat requirement is below 140 °C and moisture absorption can be designed around — PA66+GF is cheaper, processes at 280–300 °C melt temperature vs 300–320 °C, and needs a P20 or 718H tool rather than H13. PEEK when the service temperature exceeds 220 °C or the part needs to survive repeated steam sterilisation — PPS creeps above 200 °C; PEEK holds its modulus to 250 °C. PA46 when heat resistance is the main driver and cost matters — PA46 reaches 180 °C HDT, processes at 290 °C, and while it absorbs moisture more than PPS, its cost is half or less.
One subtle swap is PPS vs PPSU. PPSU is an amorphous polysulfone that processes at a similar melt temperature (330–350 °C) and mould temperature (120–140 °C), but it is transparent, tough, and survives repeated autoclaving. PPS is semi-crystalline, opaque, and brittle in thick sections without glass fibre. The tool for PPSU is similar to PPS — hardened H13 or S136, hot mould — but the part design is different because PPSU has lower shrinkage (0.5–0.7 % amorphous) and is notch-sensitive like PC.
Gestaltungsrichtlinien
- Wandstärke. Halten Sie bei den meisten Werkstoffsorten die Nennwandstärken im Bereich von 1,5 bis 3,0 mm ein; dickere Wände begünstigen Absinken und Schrumpfen, bei dünneren Wänden besteht die Gefahr einer unvollständigen Füllung. Vermeiden Sie abrupte Übergänge von dick zu dünn.
- Rippchen. Eine Rippenstärke von etwa 0,5–0,6 der angrenzenden Wand verhindert, dass die Rippe die Oberfläche eindrückt. Ordnen Sie die Rippen so an, dass die Zwischenräume zwischen ihnen gekühlt und belüftet werden können.
- Entwurf. Mindestens 1° an glatten Wänden und 1,5–2° an strukturierten Wänden. Fügen Sie an Stellen mit tiefer Prägung mehr hinzu; das Teil schleift dort am stärksten, wo die Struktur am tiefsten ist.
- Filets. Eine Verrundung mit einem Radius von mindestens 0,5 × Wandstärke an Innenecken verhindert eine Spannungskonzentration, die einen Aufprall in einen Riss umwandelt.
- Vorgesetzte. Verwenden Sie eine Wandstärke von etwa 0,6 der Nennwandstärke, fügen Sie Verstärkungsbleche hinzu, anstatt den Vorsprung zu verdicken, und halten Sie die Höhe des Vorsprungs unter etwa 2,5 × Durchmesser.
Auswirkungen auf Kosten und Durchlaufzeit
PPS sits in the middle of engineering thermoplastics on price; the premium over commodity grades buys temperature and stiffness, not a long cycle. The cost triangle is material price, cycle time and yield. A cycle that is a few seconds shorter on a high-volume part is worth more than the material saving, because the press hour is the dominant cost.
Bei der Ausbeute kann das günstige Granulat teuer werden. Feuchtes Granulat verursacht silberne Streifen und Ausschuss; eine kalte Form führt zu schwachen Schweißnähten, die im Einsatz versagen; ein schlecht entlüftetes Werkzeug verursacht Brandspuren, die Nacharbeit erfordern. Bei all diesen Punkten handelt es sich nicht um Materialkosten, und sie sind insgesamt teurer als die wenigen Prozent, die durch den Kauf einer minderwertigeren Qualität eingespart werden.
Häufige Fehler bei der Auswahl
- Verwendung eines globalen Schrumpfwerts ohne Messschleife. Die Nenntoleranz ist ein Ausgangspunkt, keine endgültige Lösung. Nehmen Sie bereits bei den ersten Messungen Korrekturen vor.
- Specifying PPS outside its temperature ceiling. Eine Betriebstemperatur, die über dem Nenn-HDT-Wert liegt, verändert das Verhalten des Bauteils über dessen gesamte Lebensdauer hinweg, selbst wenn es die Erstmusterprüfung bestanden hat.
- Das Ignorieren von Abrieb beim Befüllen des Harzes. Ein vorgehärteter Block in einer glasfaserverstärkten Form verschleißt am Anguss, lange bevor er Anzeichen von Gesamtverschleiß aufweist.
- Das TDS-Datenblatt zum Harz hinsichtlich Trocknung und Feuchtigkeitsgehalt wird nicht gelesen. Das Trocknen ist bei einer hygroskopischen Sorte unverzichtbar, und wird dieser Schritt übersprungen, führt dies zu einem Oberflächenfehler, der wie ein Formproblem aussieht.