Surface haze (often appearing as white fog or cloud-like streaks) is a common aesthetic defect, especially visible on dark, high-gloss finishes. While it may be less noticeable on white products, it is highly prominent on black or dark-colored parts.
In PP (polypropylene) products, for example, this defect manifests as irregular white streaks or cloudy patches around the part's surface. In the industry, this is classified as surface haze caused by trapped gas. You can check our full overview of common gas-related molding flaws: 16 Common Injection Molding Defects: Root Causes & Solutions

The Science Behind the Haze: Gas Trapping Explained
To fix the problem, we must understand the root cause. During the plastication phase, gaps exist between plastic pellets. As the screw rotates, it shears the material, transitioning it through three states:
- Glassy State
- High-Elastic State
- Viscous Flow State
This transformation happens in mere seconds. During this rapid process, the air trapped between pellets gets compressed into the melt. If this gas isn't properly vented from the barrel or the mold cavity, it gets injected into the part, causing gas trapping (haze) or, in severe cases, burn marks (diesel effect).
⚠️ Common Misconception: Many technicians believe that only burn marks indicate trapped gas, and their only solution is to add more venting. This is unscientific. Burn marks are simply the most extreme form of gas trapping, where compressed gas reaches temperatures of 600–800°C due to high pressure and speed, causing localized combustion. Haze is simply a milder form of the same issue. For more about venting failures that trigger haze and burns, check How Poor Venting and Mold Expansion Affect Plastic Parts.

How to Eliminate Surface Haze: Actionable Solutions
How do we ensure gas escapes without causing haze? The solution lies in balancing mold design and processing parameters.
1. Optimize Mold Venting (Don't Overdo It!)
Mold venting shouldn't be the only line of defense. PP has excellent flow properties and a wide processing temperature window. If venting slots are too large or poorly positioned, they won't help with haze and will instead cause flash defects. Precision is key.
2. Master Your Machine Parameters
Adjusting processing parameters is often the most effective way to eliminate haze. Here is how specific settings impact gas escape:
| Parameter | Recommended Action | Why It Works |
|---|---|---|
| Screw Rotation Speed | ⬇️ Decrease | Slower rotation reduces shear heat and prevents air from being folded into the melt. Fast speeds cause friction, leading to material degradation and gas generation. |
| Mold Temperature | ⬆️ Increase | Higher mold temps keep the surface molten longer, allowing for slow-fill strategies without premature freezing (which causes short shots). |
| Injection Speed | ⬇️ Decrease | Slower injection gives compressed gas time to escape through vents. Fast injection compresses gas rapidly, increasing temperature and trapping it. |
| Clamping Force | ⬇️ Decrease (Slightly) | Lower clamping force slightly improves parting-line venting. Excessive force seals the cavity too tightly, blocking gas escape. |
Many other surface blemishes like gloss unevenness share root venting and parameter issues with haze; see our full breakdown: How to Solve Injection Molding Surface Defects Like Dark Spots, Gloss Differences, and Orange Peel

Key Takeaways for Injection Molders
- Haze is trapped gas: Treat it as a venting and gas-management issue, not just a cosmetic flaw.
- Burn marks are extreme haze: Both stem from the same root cause of compressed gas.
- Slow and steady wins: Lowering screw speed, injection speed, and slightly reducing clamp force are highly effective first steps.
- Vent smartly: Ensure mold vents are correctly sized and positioned to avoid flash while allowing gas to escape.
Did this guide help you troubleshoot your injection molding defects? Share your experiences or questions in the form below!
About the Author

Alex Yu
Ideal Pro Manufacturing
Alex is the co-founder of Ideal Pro, but when he's not overseeing key projects or steering the technical team, you'll likely find him on a long bike ride, hunting for the best coffee in town, or planning his next travel adventure. With over 20 years of experience spanning international trade sales and project management, he's seen it all — tight deadlines, tricky engineering problems, and everything in between. He believes great work comes from a well-rested mind and a good cup of coffee, and he brings that same curiosity and attention to detail to every project he takes on. When he's not in the office, he's usually somewhere outdoors, exploring new places and collecting stories to share.