Reinforcement is a loan, not a gift. A 30% glass-filled grade roughly triples the flexural modulus of the base resin, and the invoice arrives later: in shrinkage that differs along the flow and across it, in warp you can only fix by moving steel, in a screw and barrel that wear several times faster, and in a process window narrow enough that a 10 °C drop in the barrel turns a good part into a short shot. Fiber-reinforced injection molding changes how the part shrinks, how the tool wears, and how the part is measured. This article works out the numbers: which loading level to buy, which defects arrive, which tolerance bands are real, and when not to use a filled grade at all.
What actually changes when you add glass to a molding resin?
Glass does not stiffen resin by being stiff. It stiffens it by carrying load the matrix would otherwise carry, and that load crosses the interface by shear, so the transfer only works if the fiber is longer than the critical length for that polymer-fiber pair. Published values for glass in polypropylene put the critical length between 1.3 and 3.1 mm, and a good coupling agent pulls it down to about 0.9 mm. Short-fiber compounds arrive already broken to 0.2 to 0.6 mm, at or below critical for many systems, which is why they act like a very stiff filler rather than a composite.
Fiber length is a process variable, not a purchasing variable. Long-fiber pellets are 10 to 25 mm in the hopper and a conventional screw delivers 1 to 3 mm at the nozzle, with the gate as the second attrition stage: a 0.8 mm pin gate on a 30% glass part shears the suspension hard at the last moment. The long-glass PP process and equipment cost breakdown shows how much of that length the plasticizing unit takes back first.
The third change is orientation, and it decides your dimensions. Fibers near the cavity wall align with the flow and freeze that way, forming a skin a few tenths of a millimeter thick; the core solidifies later with a more transverse arrangement. Fill faster into a hotter mold and the skin thickens; fill slowly into a cold mold and the core dominates. One shot therefore holds two materials with two shrinkage values, and no single number describes the part.
The property change is large enough to plan around. Unfilled PA6 sits at 2.6 to 3.0 GPa flexural modulus; the 30% glass version is commonly 9 to 10 GPa in the flow direction. Expansion along the flow falls to 2 to 4 × 10⁻⁵ per K while the transverse direction stays near 6 to 9 × 10⁻⁵ per K, and that three-to-one mismatch inside one part is a warp engine no packing pressure switches off.
Weld lines are where reinforcement stops being reinforcement. When two fronts meet, fibers lie parallel to the meeting plane instead of crossing it, so the joint is held by matrix and the few fibers that happened to bridge. On a 30% glass grade, weld-line tensile strength is commonly reported at 40 to 60% of the flow-direction value, and the scatter is worse than the mean. Put a weld in the highest-stress section and you bought a 12% part at that location.

How do you pick the loading level instead of defaulting to GF30?
GF30 is a habit inherited from metal-replacement programs, where the goal was to match a die-cast modulus and the impact requirement was already gone. It is reasonable for a structural bracket and poor for a housing that has to stay flat. The right question is not how much glass a resin will take, but what the part is failing on: stiffness, creep, heat deflection, or cost.
The table uses a PA6 base so shrinkage can be read against published figures. Modulus and shrinkage are flow-direction, dry as molded; the 10% and 35% rows are interpolated and should be confirmed with the compounder.
| Loading, PA6 base | Flexural modulus, flow | Shrinkage, flow | Shrinkage, across | Warp risk, flat part | Abrasion, screw and tool | Material cost |
|---|---|---|---|---|---|---|
| 未記入 | 2,600–3,000 MPa | 1.4–1.8% | 1.4–1.8% | 低い | Baseline | Baseline |
| 10% glass | 4,500–5,000 MPa | 0.7–1.0% | 1.0–1.4% | 中程度 | 2× | +8 to 12% |
| 15% glass | 5,500–6,000 MPa | 0.5–0.8% | 0.9–1.3% | 中程度 | 3× | +12 to 18% |
| 20% glass | 6,500–7,200 MPa | 0.4–0.6% | 0.8–1.2% | Moderate to high | 4× | +15 to 22% |
| 30% glass | 9,000–10,000 MPa | 0.3–0.5% | 0.7–1.1% | 高い | 6× | +20 to 30% |
| 35% glass | 10,000–10,800 MPa | 0.25–0.45% | 0.6–1.0% | 高い | 7× | +25 to 35% |
| 40% glass | 11,000–12,000 MPa | 0.1–0.3% | 0.5–0.9% | 高い | 8× | +30 to 40% |
| 30% glass plus mineral | 7,500–8,500 MPa | 0.3–0.5% | 0.4–0.7% | 低~中程度 | 2× | +20 to 28% |
| 40% mineral | 6,000–7,000 MPa | 0.4–0.7% | 0.5–0.8% | 低い | Near baseline | +15 to 25% |
Read the two shrinkage columns against each other, not against the unfilled row. At 30% glass the flow direction falls to a third of unfilled while the transverse direction falls only to about half, so the ratio goes from 1:1 to 1:2.5, and that ratio produces the dish after the part leaves the tool. The 40% row is sharper still, a four-to-one ratio, which is why a 40% cover is harder to hold flat than a 30% one even though it shrinks less. The shrinkage rate table by grade covers the other base polymers.
Fifteen percent is the level for less creep, less expansion and better heat deflection rather than much more stiffness: it roughly doubles modulus with the least anisotropy in the family, so a housing with a flatness call and a metal insert survives it. Twenty percent is the compromise when drop impact still matters. Thirty percent is for parts that are genuinely stiffness-limited and cannot grow a section, and the arithmetic below shows it is the cheapest modulus in the ladder; above 30% you are buying a number geometry could have supplied, since 40% glass adds about 20% modulus, costs 25 to 40% more per kilogram, and removes most remaining ductility.
Mineral fillers are the forgotten option. Talc and wollastonite are platelets and needles rather than rods, so 30% mineral reaches only 4 to 5 GPa but shrinks far more evenly and barely touches wear. For a 300 mm cover that dishes 1.5 mm, a glass-mineral hybrid at 30% total loading usually beats straight glass: you trade modulus you did not need for flatness you did.
Why does a glass-filled part shrink differently along and across the flow?
In the flow direction, fibers pack against each other and form a skeleton that resists the contracting matrix, so shrinkage is low. Across the flow the same fibers present their diameter rather than their length, the matrix pulls away, and nothing carries the contraction. Hence the familiar pair: 0.3 to 0.5% along the flow and roughly 0.7 to 1.1% across on the same 30% glass PA6, against 1.4 to 1.8% in both directions unfilled.
The consequence for toolmaking is that you cannot scale the model by a single shrink factor. The cavity is offset per direction, assuming the long axis runs with the flow, and if the molder rotates the part to fit the runner every dimension that mattered rotates with it. This is where simulation earns its fee, because it predicts the direction field instead of assuming it; the shrinkage prediction and warp simulation workflow describes what the solver needs.
Gate position is therefore a dimensional decision made at the tooling quote, not a process detail settled at first article.
| ゲートの位置 | Dimension that becomes tight | What usually happens |
|---|---|---|
| One end of a long box | Length along the flow | Length holds, width drifts wide, ends can flare |
| Center of a long part | Both halves of the length | Two fronts make a weld at the far end and a sink at the gate |
| Edge of a flat plate | Diagonal and flatness | Diagonal is fine, the plate dishes as the two directions pull differently |
| Center of a round part | Diameter and concentricity | Radial flow keeps the rim round, the center sinks |
| Into a thick rib | Rib root and the face above it | The rib packs longer than the skin, so the face shows read-through |
| Into a thin tongue | Tongue width | Gate shear aligns the skin, so blush lands on the show face |
Two numbers make the stakes concrete. A 180 mm dimension molded with the flow at 0.4% finishes at 179.28 mm; the same dimension across the flow at 1.0% finishes at 178.20 mm. That 1.08 mm difference is larger than the whole tolerance budget on most covers, and no packing profile recovers a millimeter. Decide the flow direction of the critical dimension the day you decide the gate.
Weld lines belong to this decision too: if the weld must sit on a cosmetic face, specify it and plan on texture; if it sits in a loaded section, size that section on the 40 to 60% derating.

Which defects arrive with reinforcement and what fixes them?
The defects are ones you already know, arriving for a new reason and answering to a different countermeasure. The table is ordered by how often they appear in the first week.
| 欠陥 | What produces it | First countermeasure | What the fix costs |
|---|---|---|---|
| Floating fiber, gate blush | Gate shear aligns the skin and leaves a resin-rich layer that reads as a light streak | Melt 10 to 30 °C above the unfilled setting, mold near 110 °C on PA66 with 33% glass, wider gate or fan gate | One to two days of trials, gate insert re-cut at USD 800 to 1,500, two to four weeks |
| Sink over ribs and bosses | The rib root stays molten after the skin freezes and glass does not fill the void | Rib at 0.5 to 0.6 of wall, gate closer to the rib, longer profiled pack | Tool weld and re-cut, USD 1,500 to 3,000, plus re-qualification |
| Weak or visible weld line | Fibers lie parallel to the meeting plane and cannot bridge it | Move the gate so the weld leaves the load path, or add a trimmed overflow well | Cheap before steel is cut, expensive after; a well adds a trimming step |
| Plate-out and screw wear | Sizing agents and fiber ends deposit on vents, and abrade flights and check ring | Bimetallic barrel and hardened screw, vents at 0.01 to 0.02 mm cleaned by shot count | A plasticizing unit is a five-figure replacement, see below |
| Short shot at a familiar viscosity | The fiber network adds viscosity and a yield stress the thin section must overcome | Bigger sprue and gate, higher injection pressure, melt up 10 to 30 °C, wall above 1.0 mm | Sometimes a larger machine, which is a capital decision |
| Anisotropic warp | 0.3 to 0.5% along the flow against 0.7 to 1.1% across it | Gate relocation, geometry change, mineral hybrid, or a pre-bent cavity | Cavity correction at USD 6,000 to 9,000 and three weeks |
The most expensive mistake in that table is treating a short shot as a temperature problem. A 30% glass compound is measurably more viscous at the same melt temperature than the unfilled grade, and the fiber network adds a yield stress. A 0.7 mm wall with 30% glass and 3 mm fiber is not a filling problem you tune out: it asks fibers to pass through a channel narrower than they are long. The fix is pressure and gate area, and sometimes a different grade. The defect triage order matters because the same symptom has a different first cause here, and the floating fiber and gate blush countermeasures are a procedure of their own.
Plate-out stops production at 3 a.m. Sizing chemistry migrates to mold faces and vents, and after a few thousand shots the vents blind and the part burns at the end of fill. Prevent it with a cleaning interval in the setup sheet measured in shots, and vents shallow enough that flash does not become the next problem.

What does reinforcement do to your tolerance and inspection plan?
Do not copy a tolerance table from an unfilled-part guide. Derive the band from the shrinkage window you are buying, because that window is what the molder can hold without touching steel: a 150 mm dimension in a 0.3 to 0.5% flow window has a mid-point of 0.4% and a spread of ±0.1%, which is ±0.15 mm before machine variation. A ±0.1 mm callout there is not a molding requirement, it is a request to re-cut the cavity.
| Zone of the part | Band held without a tool change | 何がそれを特徴づけているのか | How to inspect |
|---|---|---|---|
| First 15 mm around the gate | ±0.05 mm | Gate freeze and local packing | CMM or vision, mid-run part |
| Flow-direction span up to 150 mm | ±0.15 mm | Shrinkage window of the grade | CMM with the datum scheme fixed before T1 |
| Transverse span, same length | ±0.25 to 0.30 mm | Transverse window, twice as wide | CMM, with a datum face that is not the warped face |
| Weld-line zone | ±0.15 mm on position, strength derated | Two orientation fields meeting | Section or X-ray for orientation, tensile for strength |
| Flatness over a 200 mm face | 0.15 to 0.35 mm as molded | Difference between the two directions | Surface plate or functional gauge, not a caliper |
| Boss and rib positions | ±0.10 mm | Local mass and pack | CMM on five parts per shot pattern |
The plan changes shape as well as width. A caliper on a warped plate reads the high point, so a part that passes a caliper check can still fail on a surface plate, and the datum scheme has to be the one the CMM uses, on pads that are not themselves warped.
Gate-to-far-end variation is the second thing to build in. As the orifice wears, fill balance shifts and dimensions drift first in the cavities furthest from the sprue, so five parts at the start and five at the end tell you more than twenty from the middle. Where a dimension is functional, gauge it functionally: a go/no-go fixture with a center dial answers the assembly question in two seconds, and the CMM is kept for first article and capability.

What does it cost, worked out?
Four pieces of arithmetic, assumptions written in so you can substitute your own: two consumables, one on yield, one on the price of stiffness.
Start with the plasticizing unit. Assume a 90-ton machine whose screw and barrel are replaced as a set for USD 11,000 installed, that an unfilled PA66 runs 24,000 hours before flight wear and check-ring clearance make the cushion unstable, that a 30% glass grade runs about 30% of that at 7,200 hours, and that the machine runs 4,000 hours a year. Unfilled needs a set every six years, or USD 1,833 a year; glass needs one every 1.8 years, or USD 6,111 a year. Per 100,000 shots at a 30-second cycle, 833 hours of molding, that is USD 380 against USD 1,270, a gap of USD 890. A bimetallic barrel and hardened screw stretch life two to three times rather than eliminating wear, cutting the delta to a few hundred dollars.
Next, the tool. Assume a two-cavity tool with P20 gate inserts at a 1.2 mm orifice, that replacing both inserts costs USD 2,600 in EDM, polish and spotting plus two days of press downtime at USD 900 a day, so USD 4,400 per event, and that gate growth reaches 0.05 mm at 400,000 shots unfilled against 120,000 shots on glass.
| Consumable | Unfilled PA66 per 100,000 shots | 30% glass per 100,000 shots | 違い |
|---|---|---|---|
| Plasticizing unit, USD 11,000 per set | USD 380 | USD 1,270 | +USD 890 |
| Gate inserts, USD 4,400 per replacement | USD 1,100 | USD 3,667 | +USD 2,567 |
| Combined | USD 1,480 | USD 4,937 | +USD 3,457 |
Gate wear is a quality drift as well as a cost. Growing a 1.2 mm orifice by 0.05 mm adds about 8.5% flow area, enough to move fill balance between cavities by several percent and shift the weld-line position, which shows up as reject long before the gate is worn out.
Third, yield. Assume a two-cavity tool on a 26-second cycle, machine and labor at USD 48 an hour, which is USD 0.347 per cycle or USD 0.173 per part, and a 96 g shot of 30% glass PA6 at USD 3.60 a kilogram, or USD 0.346 per shot and USD 0.173 per part. Conversion cost is USD 0.346 per part. At 4% reject the cost per good part is 0.346 divided by 0.96, or USD 0.360. At 19% reject, which is what a 0.30 mm flatness call looks like on a 180 mm cover with an as-molded mean of 0.26 mm and a 0.05 mm standard deviation, it is 0.346 divided by 0.81, or USD 0.427. On 240,000 good parts a year that 15-point gap is USD 16,080. A cavity correction that pre-bends the steel by the measured 0.09 mm costs USD 7,500 and pays back in 5.6 months; if it only halves the reject rate, payback stretches to about 15 months.
Fourth, the price of stiffness. Assume a 38 g part and material at USD 3.00 a kilogram unfilled, USD 3.40 at 15% glass, USD 3.50 at 20%, USD 3.70 at 30% and USD 4.05 at 40%, with flow-direction modulus of 2,800, 5,800, 6,800, 9,500 and 11,500 MPa.
| 学年 | Material cost per part | Added cost per part | Added modulus | Cost per added MPa, per 100,000 parts |
|---|---|---|---|---|
| 未記入 | USD 0.114 | — | — | — |
| 15% glass | USD 0.129 | USD 0.0152 | 3,000 MPa | USD 507 |
| 20% glass | USD 0.133 | USD 0.0190 | 4,000 MPa | USD 475 |
| 30% glass | USD 0.141 | USD 0.0266 | 6,700 MPa | USD 397 |
| 40% glass | USD 0.154 | USD 0.0399 | 8,700 MPa | USD 459 |
Read the last column as a ladder, because the marginal steps are what you choose between. 15% to 20% buys 1,000 MPa for about USD 400 per 100,000 parts. 20% to 30% buys 2,700 MPa at about USD 280 per 100,000 parts per 1,000 MPa, the cheapest modulus in the family. 30% to 40% buys 2,000 MPa at about USD 665, roughly 2.4 times the marginal price, and takes most of the remaining unnotched impact with it. For anyone who likes round numbers the conclusion is uncomfortable: 30% is where the price curve bottoms out.
When should you NOT use a reinforced grade?
The honest cases against glass are more specific than "it gets brittle", and each has a threshold you can check against the drawing before the tool is cut.
| 要件 | Threshold where reinforcement stops paying | What to do instead |
|---|---|---|
| Unnotched impact or drop test | Any drop spec onto concrete | Test the filled grade before releasing the tool; notched impact rises while unnotched impact collapses |
| Snap fits, living hinges, press clips | Any feature that must flex beyond about 1.5% strain | Unfilled or toughened grade, or a separate spring; 30% glass breaks at 2 to 3% elongation |
| 壁が薄い | Below about 0.8 mm, especially with fiber longer than a third of the wall | Unfilled grade, or a shorter fiber and a hot mold |
| Optical clarity | Any transmission requirement | Unfilled amorphous grade; glass scatters light from the first percent |
| Painted Class A surface | Any face where read-through would print through paint | Mineral-filled or unfilled grade; paint amplifies orientation rather than hiding it |
| Dry sliding against steel | Any bushing, cam or slide running on an unhardened counterface | PTFE, aramid or silicone-modified grade, or unfilled POM; glass abrades the counterface |
| Cost-driven stiffness with room to grow the wall | When 1.5 times the wall in unfilled resin meets the stiffness target | Compare honestly: it matches stiffness but adds 53% weight and cooling time |
| Reversing fatigue across the flow | Any fully reversed load with a transverse component | Keep stress along the flow or use a mineral hybrid; transverse fatigue data is thin |
Two deserve more. The impact case is counterintuitive because datasheets suggest glass helps: notched Izod often rises from about 5 kJ/m² unfilled to 9 or 10 at 30% glass, since pulling fibers out absorbs energy, while unnotched impact, which is what a drop test measures, falls sharply because the part can no longer yield.
How do you specify a filled grade on a drawing so the molder can actually quote it?
Most filled-part quotes are wrong because the drawing lacks the information that changes the price, and the molder prices the unknown as risk. Ten callouts fix that; the CAD modeling decisions that set tooling cost belong in the same review.
| Drawing item | 何を書くか | Why the quote depends on it |
|---|---|---|
| 学年 | Base polymer, loading and a named compound such as PA6-GF30 with its grade code | Two 30% glass PA6 grades differ in impact and blush; the code pins the one you validated |
| Flow direction | An arrow on the model, plus which dimensions must run with the flow | Decides the gate, the layout and the shrink compensation |
| Shrinkage assumption | Per-direction values used to scale the model, and their source | Lets the molder check your cavity offset before steel |
| Flatness and warp zones | A value per face, with datum faces identified | Warp is the first reject driver; an unstated value becomes a dispute |
| Sink acceptance | Which faces are cosmetic and which may show read-through over ribs | Drives rib design, pack profile and polishing cost |
| Weld-line zones | Where a weld is allowed and where it is not | A weld in a seal or latch is functional, not cosmetic |
| 乾燥 | Moisture at the hopper and the drying method, as a requirement | PA6 and PA66 hydrolyze; drying is machine time and belongs in the price |
| Regrind | Percentage, passes, and whether filled regrind may be mixed | Fiber length falls every pass, so policy changes impact |
| ゲートの位置 | The agreed gate pad modeled into the part | Gate position is a dimensional decision, as the shrink section shows |
| Fiber length, long-glass grades | Pellet length and the minimum retained length expected at the gate | Length is the point of an LFT grade and the screw is where it is lost |
The two callouts that pay fastest are the flow-direction arrow and the per-direction shrink assumption: together they turn an argument about tolerance into a question about whether the model was scaled correctly, which is answerable with data. State the drying requirement too, because a 30% glass PA6 part molded wet shows splay, weak weld lines and a dimension that moves after a day on the shelf, and every symptom gets blamed on the glass.
What should you do next?
Send three things and the loading decision can be made in one review instead of three trial rounds: the model with the gate area and cosmetic faces marked, the function with a number attached to it — a stiffness, a flatness, a drop height, a creep limit — and the annual volume with the target piece price. From those, the grade ladder, the gate position and the tolerance bands can be fixed before the cavity is cut, which is the only point where any of them is cheap to change. Our mold-making stage gates before steel is cut list the checkpoints for signing each one off.
- Email: [email protected]
- Phone and WhatsApp: +86 156 0682 1288
よくある質問
ガラス繊維含有率30%の材料は、40%の材料よりも強度が高いのでしょうか?
ガラス繊維強化プラスチックは、非強化プラスチックに比べて収縮率が高いですか、それとも低いですか?
無充填樹脂用に設計された金型で、ガラス充填グレードを成形することは可能ですか?
ガラス繊維強化部品が、なぜ溶接線部分で割れてしまうのでしょうか?
Do I need a special screw and barrel for glass-filled resin?
著者について

アレックス・ユー
アイデアル・プロ・マニュファクチャリング
アレックスはIdeal Proの共同創業者ですが、重要なプロジェクトの監督や技術チームの指揮をとっていないときは、長距離サイクリングを楽しんだり、街で一番おいしいコーヒーを探し回ったり、次の旅の計画を立てたりしている姿を見かけるでしょう。 国際貿易の営業やプロジェクト管理に20年以上の経験を持つ彼は、厳しい納期や厄介な技術的課題など、ありとあらゆる状況を経験してきました。彼は、素晴らしい仕事は十分な休息と一杯の美味しいコーヒーから生まれると信じており、その好奇心と細部へのこだわりを、手掛けるすべてのプロジェクトに注ぎ込んでいます。 オフィスにいないときは、たいてい屋外で、新しい場所を探索したり、皆と共有できるエピソードを集めたりしています。.